Article

C36000 vs C3604: Which Grade Designations Actually Transfer

A US drawing says C36000; the bar on the rack in Taiwan certifies to C3604, and a bar inside the JIS limits can sit outside the ASTM ones. This article covers which of five common grades transfer, which are only close, and which numbers on the mill certificate answer it.

One pair matches, three are close, and one has no UNS number

Your quality system checks the mill certificate against the grade on the drawing, and in my experience the certificate that comes with bar bought in Taiwan is written to JIS. For some pairs that makes no difference. For others, a bar that passes JIS can fail the ASTM grade on copper.

Aluminum 6061 and 6063: the JIS limits match the Aluminum Association limits on every element I can check. Free-cutting brass C36000 and C3604: the closest grades to each other, not equivalents; the copper windows barely overlap. Carbon steel 1045 and S45C: close, with different carbon, phosphorus and sulfur limits. Free-machining steel 12L14 and 1215: JIS SUM24L and SUM23 match on carbon, manganese and phosphorus, with sulfur and lead still to be read off a certificate. Lead-free bismuth brass C6801: no UNS number to translate into.

C36000 and C3604 are the closest grades to each other, not equivalents

Many supplier tables treat them as the same alloy, but the two specifications set different limits.

ASTM B16/B16M C36000: copper 60.0 to 63.0 percent, lead 2.5 to 3.0 percent, iron 0.35 percent maximum, zinc the remainder. Editions of B16 before 2010 allowed lead up to 3.7 percent, a figure some supplier tables still print.

JIS H3250 C3604: copper 57.0 to 61.0 percent, lead 1.8 to 3.7 percent, iron 0.50 percent maximum, zinc the remainder.

Every C36000 lead value is also a C3604 lead value. The copper windows share one percentage point, 60.0 to 61.0.

So a C3604 bar with copper below 60.0 percent is inside JIS and outside C36000, even when its lead sits in the 2.5 to 3.0 percent range both grades accept. In that case lead, usually the first number checked, does not tell the two grades apart.

I went through the C3604 certificates I have on file. There are eight, from two suppliers, the earliest dated 2022. Copper reads 58.2 to 58.5 percent on every one. Lead reads 2.65 to 2.72 percent.

Whether that matters is a design question for your part. But if your drawing says C36000 per ASTM B16 and your quality system checks the certificate against that, a C3604 certificate fails the check. Either the drawing accepts C3604 by name, or the shop orders bar certified to C36000. Bar certified to C36000 can be ordered in Taiwan; ask at the quoting stage which certificate the shop will supply, and whether price, lead time or minimum quantity changes with it.

Lead-free brass has no clean cross-reference

JIS H3250 carries a group of bismuth free-cutting brasses. One of them is C6801: copper 57.0 to 64.0 percent, bismuth 0.5 to 4.0 percent, lead 0.01 percent maximum, zinc the remainder. A C6801 certificate I have on file shows 1.88 percent bismuth and 0.0053 percent lead.

I also have certificates for a second bismuth brass bar. They state a lead limit under 0.1 percent and show 0.017 to 0.044 percent. That is a different grade from C6801, whose limit is 0.01 percent.

UNS has bismuth brasses too, under ASTM B974. Two of them are C49250, with bismuth 1.8 to 2.4 percent, and C49260, with bismuth 0.50 to 1.8; both cap lead at 0.09 percent. C6801 allows bismuth anywhere from 0.5 to 4.0, wider than both together. The silicon brass C69300 is a different alloy system again. None of these is C6801 under another name, and I have not found any standards body that treats them as equivalent.

So when a US drawing says "lead-free brass" and a Taiwanese shop quotes C6801, there is no table to check against, only the certificate: copper, zinc, bismuth and lead against whatever your own specification says the wetted material has to be. If the drawing names a specific UNS grade, C6801 is a substitution and needs your written approval before the bar is cut.

"Lead-free" also means two different things here. For C6801, the JIS limit is lead 0.01 percent maximum in the bar. "Lead free" under the US Safe Drinking Water Act means a 0.25 percent weighted average over the wetted surfaces of the finished product, with third-party certification generally required since September 2023. The JIS number is about the bar. The US rule is about the finished product, and that is a question for a compliance professional, not something a mill certificate can answer.

Aluminum 6061 and 6063 are the easy case

6061 and 6063 are Aluminum Association designations, and the JIS limits I can find for A6061 and A6063 match them element for element. UNS calls them A96061 and A96063, the same number with a prefix.

6061: silicon 0.40 to 0.8, iron 0.7 maximum, copper 0.15 to 0.40, manganese 0.15 maximum, magnesium 0.8 to 1.2, chromium 0.04 to 0.35, zinc 0.25 maximum, titanium 0.15 maximum.

6063: silicon 0.20 to 0.6, iron 0.35 maximum, copper 0.10 maximum, manganese 0.10 maximum, magnesium 0.45 to 0.9, chromium 0.10 maximum, zinc 0.10 maximum, titanium 0.10 maximum.

The temper does not carry over by itself. Chemistry and temper are separate lines on the certificate: if the drawing needs T6, say T6 and look for it on the certificate.

12L14 and 1215 are free-machining steels with a lead question attached

The main difference between them is one element.

12L14, UNS G12144: carbon 0.15 maximum, manganese 0.85 to 1.15, phosphorus 0.04 to 0.09, sulfur 0.26 to 0.35, lead 0.15 to 0.35.

1215, UNS G12150: carbon 0.09 maximum, manganese 0.75 to 1.05, phosphorus 0.04 to 0.09, sulfur 0.26 to 0.35, no lead.

In my experience, Taiwanese shops buy these under the US names more often than under JIS grades. The 12L14 certificates I have on file are written to SAE J403, not to a JIS number, and lead reads 0.29 and 0.30 percent. The JIS free-cutting group is the SUM series in JIS G4804. SUM24L corresponds to 12L14 and SUM23 to 1215, and they are identical on carbon, manganese and phosphorus. If a certificate does say SUM24L, read the sulfur and lead off the composition table.

12L14 is a leaded steel and 1215 is not. If the part has a lead limit and the drawing says 12L14 out of habit, 1215 is the substitution to ask about.

1045 and S45C are close, and the difference is at the edges of the carbon window

1045 (ASTM A29): carbon 0.43 to 0.50, manganese 0.60 to 0.90, phosphorus 0.040 maximum, sulfur 0.050 maximum.

JIS G4051 S45C: carbon 0.42 to 0.48, manganese 0.60 to 0.90, phosphorus 0.030 maximum, sulfur 0.035 maximum.

S45C is the tighter specification on phosphorus and sulfur. The carbon windows overlap but are not identical: a bar at 0.49 or 0.50 percent carbon is 1045 and not S45C; a bar at 0.42 is S45C and not 1045. On a turned part that is not heat treated, this rarely matters. On a part hardened to a specification, check the hardness on the first Taiwanese lot rather than assume it.

The numbers to check are the measured values, not the grade name

In every case above, start with the chemical composition table on the mill certificate. The certificates I handle give two values per element: the specification range and the measured value for the bar. Read the measured value against the limits of the grade your drawing names, not against the limits printed on the certificate. On the certificates I handle the specification row says JIS, and your drawing says ASTM. The measured numbers are the same whichever standard you check them against.

While you are there, the heat or report number on the certificate should match the one on the bar tag and, if your order calls for it, on the shipping documents.

How to write the material line so a Taiwanese shop can quote it honestly

Name the grade and the standard, then say what you will accept. "C36000 per ASTM B16" is a different request from "C36000 or JIS C3604": the first needs bar ordered against a C36000 certificate, the second also accepts a certificate that says C3604.

For lead-free brass, name the limit rather than the grade unless the grade is genuinely required. "Pb 0.25 percent maximum in the bar, bismuth brass acceptable" is a line a Taiwanese shop can meet with a certificate; "C69300" names one silicon brass, and a shop quoting bismuth brass against it is quoting a substitution.

For aluminum, write the temper. For free-machining steel, say whether lead is acceptable. For 1045, say whether S45C is acceptable and whether the part is heat treated.

And ask for the certificate at the quoting stage, not at shipment. A recent certificate for the grade the shop intends to use shows you which standard it is written to before any bar is ordered.

This is general information about material standards and how a mill certificate is read, not engineering or compliance advice for a specific part. Composition limits are summarized from the standards named in the text; check the current edition of each before relying on a figure. Confirm any substitution with your own engineering and, where a product regulation applies, with a compliance professional.

Sean Shih is the founder of Celvor Industrial in Taichung, Taiwan.

If you are sourcing a turned part in any of these grades, send the drawing.